Both processes give a hard, wear-resistant surface on a tougher core. They get there in very different ways. The choice affects which steel you buy, how much you grind after heat treatment, where the heat-treatment step sits in your plant, and how much distortion you have to correct.
This guide compares induction hardening with carburising, the most common case-hardening route for gears and shafts.
How each process works
Induction hardening heats only the zone that needs to be hard. A water-cooled copper coil carries an alternating current. The current induces eddy currents in the surface of the part, and the surface heats in seconds. A spray or immersion quench follows straight away. The hard layer is martensite formed from the steel’s own carbon. Nothing is added to the steel.
Carburising changes the chemistry of the surface. The part is held in a carbon-rich atmosphere in a furnace. Gas carburising is normally done at 900–950 °C. Carbon diffuses into the surface over a period of hours. The part is then quenched, so the high-carbon surface forms martensite while the low-carbon core stays tough.
The key difference: induction relies on carbon already in the steel. Carburising adds carbon to a steel that does not have enough.
Steel selection
This is usually where the decision starts.
- Induction hardening works best on medium- and high-carbon steels and on medium-carbon alloy steels. The steel must already contain enough carbon to reach the hardness you want.
- Carburising is used on low-carbon steels. These steels would not harden enough by themselves.
So you cannot take a drawing written for a carburising steel and simply send the part to an induction line. If you want to change process, the steel grade normally changes too. Treat the induction steel with the same care as a carburising steel: check composition, grain size and cleanliness, not only the hardenability.
Case depth
| Induction hardening | Carburising | |
|---|---|---|
| Typical case depth | About 0.5–5 mm | Several millimetres possible, set by time at temperature |
| What sets the depth | Frequency, power and heating time | Temperature, carbon potential and time |
| Where the case is | Only where the coil heats | Everywhere exposed to the atmosphere, unless masked |
Induction gives selective hardening. You can harden a bearing seat and leave a thread or a weld area soft. With carburising you mask the areas that must stay soft, or machine the case off later.
For a guide to matching frequency with case depth, see our article on choosing an induction heating frequency.
Distortion and grinding
Carburising holds the whole part at high temperature for a long time and then quenches it. This tends to cause more distortion. Many gear makers use press quenching to control it. After heat treatment the part is ground to size, and grinding removes some of the hardest layer with the highest compressive stress.
Induction heats a smaller volume for a much shorter time. Distortion is usually smaller. Because the induction case is often deeper than a carburised case, the same grinding stock removes a smaller share of it. That gives more freedom in setting grinding allowances.
Distortion still happens with induction. Uneven heating, a coil that is off-centre, or a part with very different wall sections will move. Coil design and part support matter.
Cycle time and plant layout
| Induction hardening | Carburising | |
|---|---|---|
| Heating time | Several seconds to tens of seconds per part or zone | Hours per furnace load |
| Flow | One part at a time, in line with machining | Batch, often in a separate heat-treatment shop |
| Fixtures | Coil (inductor) made for each part geometry | Baskets and fixtures; one load can hold many parts |
| Start-up | Power on and run | Furnace and atmosphere need time to stabilise |
Induction fits well into a machining cell. Parts come off the lathe, are hardened, and move on. Carburising fits a central heat-treatment shop that handles large batches of mixed parts.
Where induction does not fit well
Induction is not the answer for every hardened part. It is usually a poor choice for:
- Complex sections. A transmission shaft with several gears, steps and bearing seats close together is hard to heat evenly with one coil. Sharp corners in the hardened zone overheat.
- Thin walls. The heat can pass right through a thin section. The whole wall then hardens and may crack.
- Very small parts in high volume. Each part must be loaded, heated and quenched on its own. A carburising furnace can treat thousands of small parts in one load.
- Single pieces and very small batches. Each new geometry needs its own coil. The coil cost is hard to recover on a few parts.
Where carburising does not fit well
- Parts that need a hard zone only in one place, with the rest left soft for machining or welding.
- Large parts where furnace size, handling and distortion become the main cost.
- Production lines that cannot wait for batch furnace cycles.
Prior heat treatment matters for induction
Induction heating is short. The steel has little time to even out its structure during the cycle. Start from a uniform structure, usually normalised or quenched and tempered. A banded or coarse starting structure gives uneven hardness and a patchy case. The core properties come from this prior treatment, not from the induction step.
Summary: a quick decision guide
| If the part… | Lean towards |
|---|---|
| Is a medium-carbon steel and needs a hard zone in one area | Induction |
| Is a low-carbon steel and needs a hard surface all over | Carburising |
| Has a simple shape repeated in volume (shafts, pins, gear teeth, races) | Induction |
| Has many close steps and sharp corners in the hard zone | Carburising |
| Is very small and made in very large numbers | Carburising |
| Must be hardened in line with machining | Induction |
Many plants use both. The right answer depends on the part, the steel and the volume.
Send us the drawing, material and target case depth, and our engineers will recommend a frequency and power.
Sources
- JKZ (old site): Differences between induction hardening and case hardening — Induction case depth typically 0.5–5 mm; induction cycles in seconds, carburising in hours; steel suitability for each process
- JKZ (old site): Economic analysis of induction quenching — Induction heating time of several seconds to tens of seconds; grinding stock and case depth after heat treatment
- JKZ (old site): A proposal for substitution of induction hardening for carburizing — Limits of induction hardening: complex sections, sharp corners, thin walls, very small parts, single pieces; importance of prior heat treatment and steel quality
- JKZ (old site): Indicators of induction hardening technology — Carburising at high temperature for a long time gives larger quench distortion; induction distortion is smaller
- Wikipedia: Carburizing — Carburising is applied to low-carbon steel; gas carburising is normally done at 900–950 °C; non-uniform sections can crack from uneven cooling