Induction hardening defects: cracks, soft spots, uneven case, overheating and prevention

Causes of the common induction hardening defects and the checks on steel, coil, quench and tempering that prevent them on the production line.

Updated 1 October 2026 · 6 min read

Most induction hardening defects come from a small set of causes: too much heat in one place, too little heat in another, a quench that does not reach every part of the surface, or a steel that was not ready for hardening. This guide groups the common defects by symptom, then lists the checks that prevent them.

Quench cracks

Cracks are the most serious defect because the part is scrap and the crack may not be found until it fails.

Where they start. Cracks usually start where heat concentrates: sharp corners, the edges of keyways, oil holes, cross holes and sudden changes in wall thickness. The induced current crowds into these edges, the metal overheats, and the quench then sets up high stress at the same spot.

Main causes:

  • Overheating, or a temperature that is uneven across the zone
  • A quench that is too severe for the steel
  • Carbon content. Crack risk is low with steel near 0.30% carbon and much higher near 0.50% carbon
  • A poor starting structure: coarse grain, segregation, inclusions or slag
  • Tempering that is late or not enough

Prevention:

  • Add radii to sharp edges where the drawing allows it.
  • Plug holes and keyways with copper inserts during heating. The copper carries the current around the opening and stops the edge from overheating.
  • Choose a quenchant with a moderate cooling rate for crack-sensitive steels. Polymer (PAG) solutions are common for this.
  • Temper as soon as possible after hardening.
  • Ask for a normalised or quenched-and-tempered starting structure from your steel supplier or your own prior heat treatment.

Soft spots and soft bands

A soft spot is an area in the hard zone with low hardness. On scan-hardened shafts it often shows as a spiral band of discoloured metal. Light grinding removes the colour but not the soft metal underneath.

Main causes:

  • Blocked or badly sized holes in the spray ring. Some of the surface does not get enough quenchant, quickly enough.
  • Dirt or scale in the quench water
  • A coil-to-part gap that varies around the part
  • A starting structure with network carbides or coarse spheroidised carbides that do not dissolve in the short heating time
  • Scan speed or power that does not match the part, so some areas never reach hardening temperature

Prevention:

  • Inspect and clean the spray ring on a schedule. Check that every hole is open.
  • Filter the quenchant. Keep the tank clean.
  • Check the coil gap and the part centring. A guide or float device on the machine helps hold the gap.
  • Check concentration of polymer quenchant with a cooling-curve test, not only with a refractometer. The polymer degrades in use and the refractometer reading can stay the same while cooling performance changes.

Uneven or shallow case

The case depth varies around the part, or is shallower than the drawing.

Main causes:

  • Coil design that puts too much power in one area and too little in another
  • Wrong frequency for the depth. Frequency is the main factor that sets case depth. See our guide on choosing a frequency.
  • Power too low for the scan speed, or scan speed too high for the power
  • A banded structure or partial decarburisation in the steel
  • A worn or deformed coil

Prevention:

  • Section and etch a sample part when you set up a new coil, and repeat on a schedule.
  • Keep a record for each coil. Note its date into service, any reshaping or repair, and the case-depth results it produces. Retire coils that drift.
  • If the coil carries magnetic flux concentrators, repair them correctly. Laminated concentrators need their insulation restored after reshaping. Ferrite concentrators are brittle and crack under force.

Overheating, burning and surface melting

The surface shows coarse grain, scaling, pitting or local melting.

Main causes:

  • Heating time too long
  • Coil too close to the part, or touching it at one point
  • Sharp corners, holes or existing surface cracks that concentrate the current
  • Poor coil design

Prevention:

  • Set and check the coil gap at every changeover.
  • Protect holes and keyways as for crack prevention.
  • Lock heating time and power in the recipe so operators cannot extend them.

Peeling or spalling of the case

The hard layer flakes off in service. This points to a very steep change in hardness between the case and the core.

Prevention: use a short induction preheat before the hardening shot to make the transition more gradual, and start from a quenched-and-tempered structure so the hardening penetrates more evenly.

Grinding cracks and grinding burn

These defects appear after hardening, during finish grinding. Local grinding heat re-tempers or re-hardens the surface.

  • Cracks that form at about 180 °C appear as parallel lines across the grinding direction.
  • Cracks that form at about 250–300 °C appear as a network.

Higher hardness, more carbides and steels containing chromium and molybdenum all make more grinding heat. Prevention is on the grinding side: wheel selection, dressing, coolant and feed rate. Hot acid etching shows grinding cracks.

Tempering after induction hardening

Temper soon after hardening. Two methods are common on induction lines:

  • Self-tempering. The quench is stopped early. Heat left in the core flows back to the surface and tempers it. This suits simple parts hardened in one shot.
  • Induction tempering. A second coil, after the quench, reheats the hardened zone at lower power. This suits shafts and sleeves on a continuous line.

Furnace tempering is also used, especially when the plant already has a tempering furnace.

Quick reference

Defect First things to check
Cracks Edges and holes, quench severity, carbon content, time to temper
Soft spots Spray holes, quenchant condition, coil gap
Uneven case Coil condition, frequency, power and scan speed
Overheating Heating time, coil gap, sharp features
Peeling Hardness gradient, prior structure

Send us the drawing, material and target case depth, and our engineers will recommend a frequency and power.

Sources

  1. JKZ (old site): Detailed explanation of high-frequency quenching defects and prevention — Crack causes; crack risk low near 0.30% carbon and high near 0.50% carbon; soft spots; burns; grinding cracks near 180 °C and 250–300 °C
  2. JKZ (old site): Common problems and solutions of high-frequency quenching — Overheating at corners, keyways and holes; copper inserts; soft bands from blocked spray holes; peeling from a steep hardness gradient
  3. JKZ (old site): Common quality problems of induction quenching machine — Causes of cracking, uneven hardness and surface melting; prior normalising or quench and temper; prompt tempering
  4. JKZ (old site): Quality control of induction hardening — Coil-to-part gap control; inductor records; PAG quenchant monitoring by cooling curve; power and scan speed matched to the part
  5. JKZ (old site): Several commonly used tempering methods in induction quenching — Self-tempering and induction tempering after induction hardening

Send us your part.

We reply within 1 working day.

Our timeUTC+8

[email protected]+86-28-84211110